CEMENT BASED GREY THICK REPAIR MORTAR FORMULATION AND PRODUCTION PROCESS
CEMENT BASED  GREY THICK REPAIR MORTAR FORMULATION AND PRODUCTION PROCESS
CEMENT BASED  GREY THICK REPAIR MORTAR FORMULATION AND PRODUCTION PROCESS CEMENT BASED  GREY THICK REPAIR MORTAR FORMULATION AND PRODUCTION PROCESS
PORLAND GREY CEMENT ( 42.5 r )

SILICA SAND ( 100 - 300 )

DOLAMITE ( 5 - 10 MICRON )

HYDROXYETHYL CELLULOSE ( HEC )
374

550

75

1

CEMENT BASED  GREY THICK REPAIR MORTAR FORMULATION AND PRODUCTION PROCESS CEMENT BASED  GREY THICK REPAIR MORTAR FORMULATION AND PRODUCTION PROCESS CEMENT BASED  GREY THICK REPAIR MORTAR FORMULATION AND PRODUCTION PROCESS


CEMENT BASED  GREY THICK REPAIR MORTAR FORMULATION AND PRODUCTION PROCESS

PROCESS: In the above ingredients are solid and powder. So, Charge all ingredients in the mixing tank. Start to mix. Continue to stirr until mixture is homogenous. Homogenous is enough. Process is completed.
 
 
 
NOTE: Amount of ingredients used above formulation can be changed depending condition of market.



NOTE: Above formulation is taken from CONSTRUCTION CHEMICALS FORMULATIONS ENCYCLOPEDIA - 1 

 